Tech nical
specifications for H.D PE
100 , PE 80
 

 
Test
Conditions for Follow -Up
Testing
| PE
80 |
PE
100 |
| proof
stress, s0 in
N/mm2 |
Time
to failure, t, in
hours |
proof
stress, s0 in
N/mm2 |
Time
to failure, t, in
hours |
| 4.6 |
165 |
5.5 |
165 |
| 4.5 |
219 |
5.4 |
233 |
| 4.4 |
293 |
5.3 |
332 |
| 4.3 |
394 |
5.2 |
476 |
| 4.2 |
533 |
5.1 |
688 |
| 4.1 |
727 |
5.0 |
1000 |
| 4.0 |
1000 |
|
|
| Test |
PE
100 |
PE
80 |
| Density
G/CM2 |
0.95 |
0.94 |
| M.F.R
( 2.16 KG / 10
Min) |
0.2G
/ 10 Min |
0.4G
/ 10 Min |
| Tensile
N / MM2
|
>=20 |
>=14 |
| Elongation
0/0 |
>=500 |
>=350 |
| O.I.T |
>=20
Min at 210 c |
>=
20 Min at 200 c |
Test
conditions for hydrostatic
pressure testing
Material
Designation
| Material
designation |
Minimum
required
strength*) MRS in
N/mm2 |
| PE
80 |
8.0 |
| PE
100 |
10.0 |
| PE-HD |
- |
| *)
see DIN EN
ISO 12162
for definition. |

| Material |
Test
Teperature in C |
Proof
stress 0 in N/mm |
period
of stressing
(minimum time to
fallure) t, in
houre |
| PE
80 |
20
80
80 |
10.0
4.6
4.0
|
100
165
1000 |
| PE
100 |
20
80
80 |
12.4
5.5
5.0 |
100
165
1000 |
|